Ferro molybdenum is an alloy composed of iron and molybdenum. It serves as a hardening agent in many alloy steels. Molybdenum prevents corrosion in stainless steel and, when mixed with iron, also hardens and strengthens it into austenite. Ferro molybdenum is produced by heating/melting a mixture of molybdenum oxide and iron. It can be produced in induction/arc furnaces or through aluminum thermal reactions. It’s added to the steel melt before casting. There are various grades of ferromolybdenum, but the molybdenum content mostly varies between 60 – 75%. It’s not classified as a hazardous material for transportation. Nearly 80% of the global ferromolybdenum production comes from China, the United States, and Chile.
Ferro molybdenum is used in steelmaking to manufacture alloy steels suitable for mining and refining, military hardware, rotary drills, and load-bearing components. FeMo is also used in stainless steels, heat-resistant steels, and tool steels.


Ferromolybdenum production process
Ferromolybdenum production process using out-of-furnace method
1. Raw Material Production for Ferro molybdenum
- Rhenium molybdenite is the main raw material for ferromolybdenum production and serves as the source of molybdenum in ferromolybdenum. It has strict requirements for impurities besides demanding high grades. General composition: Mo 48%-52%, S ≤ 0.065%, P ≤ 0.023%, Cu ≤ 0.30%, SiO2 8%-14%, Pb 0.2%-0.5%. The particle size should not exceed 20mm, with 10-20mm particles not exceeding 20% of the total.
- Ferrosilicon powder is a powdered raw material made from 75% ferro silicon through crushing and ball milling, used for reducing molybdenite, iron scales, and other oxides. Before use, ferro silicon powder must undergo accurate silicon and aluminum content analysis, with silicon content ranging from 75%-77%, and particle size requirements: not exceeding 1.0-1.8mm by 1%, and not exceeding 10% for particle sizes of 0.5-1.0mm, with the rest below 0.5mm. Large particle sizes can cause an increase in silicon content in ferromolybdenum, and ferrosilicon powder with higher silicon content performs better than lower silicon content.
- Aluminum granules should have accurate aluminum content as a basis for ingredient calculation, with particle size requirements below 3mm. Particle sizes too small are unsafe during production, while too large sizes are unfavorable for smelting reactions. The amount of aluminum granules added depends on the temperature, molybdenum content, production scale, and temperature conditions of the molybdenite, generally adding 5-8kg per batch.
- Iron scales are oxide scales during steel rolling and forging, serving as an oxidant and flux in smelting. About 30% of iron scales enter the alloy during smelting, being one of the sources of iron in the alloy; about 70% of iron scales enter the slag in the form of FeO, diluting the slag. Requirements for iron scales: Fe ≥ 68%, S ≤ 0.05%, P ≤ 0.035%, C ≤ 0.30%, Cu ≤ 0.1%. Iron scales need to be heated and dried to remove moisture and oil before use, and iron ore can also be used in production, but iron ore has higher sulfur content and is rarely used domestically.
- Steel scraps are the main source of iron in the alloy, requiring iron content greater than 98%, generally using carbon steel scraps. Fluorite particle size should be below 20mm, heated and dried before use to remove moisture, with CaF content in fluorite ≥ 90%, S ≤ 0.05%, and P ≤ 0.05% to be usable. The amount of fluoride added to the charge depends on the actual slag conditions and the SiO2 content in the molybdenite, generally adding 2-3kg per batch.
- Saltpeter is sodium nitrate, used as a reheating agent when low-molybdenum molybdenite is used, often due to insufficient oxygen and cannot be increased in reducing agents, resulting in low heat generation of the charge. Each batch of material is supplemented with 1-3kg.
Ferromolybdenum charge ratio
The charge ratio is 100kg of molybdenite; 3kg of saltpeter; 6kg of aluminum granules; 20kg of iron scales; 28.28kg of ferrosilicon powder; 23.06kg of steel scraps; 2kg of fluorite; totaling 182.34kg.
The total heat release per batch is:
102195.6 + 266662 + 17170 + 8716.9 + 25288.3 = 420032.8 (kJ)
2. Ferro molybdenum Smelting Operation
Preparation of Charge Materials
The charge materials should be processed into suitable particle sizes, then dried and mixed according to the ingredient ratio. Accurate weighing of the charged materials is a prerequisite for ensuring normal smelting. The order of weighing is molybdenite, saltpeter, aluminum granules, iron scales, ferrosilicon, steel scraps, and fluorite. The weighed charge materials are mixed in a mixing machine for about 8 minutes until uniform, then transferred to a charging hopper.
The charging work is a very careful task, with no room for error. The charging personnel should be focused and responsible. The use of electronic control devices is preferred whenever possible.
Fire prevention measures should be strictly implemented during charging due to the flammability of the charged materials and the explosiveness of dust. The mixing process should be equipped with tight sealing and smoke exhaust and dust removal facilities.
3. Ferromolybdenum raw materials are added to the furnace
The furnace is the main equipment for smelting ferromolybdenum. The furnace shell is a circular cylinder made of 10mm steel plate, lined with refractory clay bricks, with a 120mm diameter slag tapping port set 100mm above the bottom edge of the furnace shell. The furnace is placed on a sand base, with a hemispherical pit made in the sand base to accommodate the molten alloy. The pit for accommodating the alloy is called the sand pit.
Dried river sand is used to make the sand pit. After the furnace cylinder is placed, the sand pit is compacted, especially the joint between the lower edge of the furnace cylinder and the sand pit, which should be compacted to a height of 150-200mm inside and 400mm outside to prevent slag from leaking out of the joint during smelting. The sand pit is naturally dried, and wet sand pits are strictly prohibited to prevent serious splashing and even injury.
4. Ferro molybdenum Smelting
The well-mixed charge materials are loaded into the furnace. After the first batch is added, precise returns and fragments are added, forming a hollow circle, avoiding close contact with the furnace wall to prevent bonding to the furnace wall without melting and ensuring there is no interruption in the reaction. After the circular layout, the second batch of charge materials is added, and after the charge materials are loaded, the surface of the charge should be no less than 500mm from the upper edge of the furnace to prevent splashing during the reaction.
A pit is made in the center of the charge surface, and an ignition mixture is added, then a steel rod is inserted into the ignition material and shaken, allowing the ignition material to communicate with the lower charge. Magnesium shavings, 100g, are added to the center of the ignition material, and the smoke hood is positioned properly before igniting with a red-hot rod, and the reaction proceeds automatically.
The changes in the reaction process spread from the center downward and outward. The normal reaction time is less than 10 minutes. The reaction is gentle in the first quarter of the time, intense in the middle period, emitting a large amount of brown smoke, boiling, and slight splashing, and slows down in the last quarter, with bright flames, lighter smoke, and a noticeable bright end to the reaction.
The normal signs of the smelting process
- The reaction is intense, emitting thick smoke without interruption, no splashing, and a clear end to the reaction. After the reaction, the smoke becomes bright and transparent.
- When tapping slag, the slag has good flowability with slight bonding. After cooling, the surface of the slag in the slag pot protrudes and has a glossy surface, with the slag appearing dark green.
- When lifting the furnace cylinder, there is a pulling slag wire phenomenon, and the slag cover on the ferromolybdenum ingot is slightly concave.
- The reaction time is within the range of 2-10 minutes.
Abnormal phenomena, causes, consequences, and handling methods during the smelting process are as follows
- Other phenomena are normal, but there is a large amount of splashing. This is caused by moist charge materials or excessive unit heat generation. This phenomenon easily leads to furnace leakage or splashing of charged materials, resulting in high silicon content in the alloy. If the unit heat generation is too high, reduce the aluminum granules and increase the amount of ferrosilicon powder added; if the charge materials or sand pits are wet, solve the drying problem of the charge materials and sand pits.
- The reaction is too intense, with a large amount of splashing, a short reaction time, and a quick end; after the end, the smoke is bright, the slag is sticky, and the color is blue-green. Small molybdenum iron samples taken out after cooling are easily fragmented, with a bright silver-white appearance on the fracture surface. This is a manifestation of an excessive reducing agent, often resulting in high silicon and low molybdenum in the alloy. In this case, reduce the amount of reducing agent added, generally by 0.3-0.7kg per batch.
- The reaction is stable, with intermittent reaction, dark brown smoke rising slowly. The reaction time is long, with an unclear and prolonged end. After lifting the furnace, bubbles appear on the slag surface of the ferromolybdenum ingot, and fire is emitted. After cooling, small molybdenum iron samples taken out have black-brown slag adhering to the surface, and the molybdenum iron samples are very hard, with uneven fracture surfaces, appearing gray-black. This is a manifestation of an insufficient reducing agent. This can lead to a high molybdenum content in the alloy, low silicon content (less than 0.05%), layering of ferromolybdenum ingots, rusting during cooling, difficulty in refining, high molybdenum content in the slag, and more metal particles. In this case, increase the reducing agent, generally by adding 0.2-0.5kg per batch.
- The reaction proceeds slowly, with no obvious normal smoke, and a long reaction time. This is due to insufficient heat generation of the charge materials. This often results in high molybdenum and silicon content in the alloy, and the iron ingot is layered or segregated. The 30 minutes after the end of the reaction is the settling time for metal particles to ensure that the molybdenum content in the slag is below 0.35%. Open the slag tap, and the slag flows into the slag pot, and samples are taken to analyze the molybdenum content. Rich slag above 0.35% must be returned for smelting. Poor slag can be discarded or comprehensively utilized. After tapping the slag, lift the furnace cylinder and use an iron spoon to take iron samples from the metal ingots on the sand base. The alloy surface is smooth, with a slight green slag, a dense silver-gray fracture surface, fine crystals, and no bright spots, indicating good quality molybdenum iron. The normal range of alloy and slag composition is as follows.
After the end of the reaction, the settling time for metal particles is 30 minutes to ensure that the molybdenum content in the slag is below 0.35%. Open the slag tap, and the slag flows into the slag pot, and samples are taken to analyze the molybdenum content. Rich slag above 0.35% must be returned for smelting. Poor slag can be discarded or comprehensively utilized. After tapping the slag, lift the furnace cylinder and use an iron spoon to take iron samples from the metal ingots on the sand base. The alloy surface is smooth, with a slight green slag, a dense silver-gray fracture surface, fine crystals, and no bright spots, indicating good quality ferromolybdenum. The normal range of alloy and slag composition is as follows.
| Ferromolybdenum composition | Mo | Si | C | S | P | Cu | Su | Sb | As | Pb |
| % | 59-61 | 0.5-1.0 | 0.05-0.10 | 0.05-0.08 | 0.03-0.04 | 0.1-0.5 | 0.01-0.04 | 0.01-0.04 | 0.01-0.02 | 0.0001-0.005 |
| Slag composition | Mo | SiO2 | MgO | Al2O3 | FeO | CaO | S | |||
| % | 0.01-0.35 | 58-63 | 1.0-2.0 | 11-15 | 16-24 | 3-5 | 0.01-0.03 |
5. Composition of Ferro molybdenum Alloy and Slag
The ingots are cooled in the sand pit for 7-8 hours and lifted with special tools. The sintered sand layer at the bottom of the ingot should be scraped off, and the slag cover on the upper part of the ingot should be removed with a rake, and then compressed air is used to blow off the molten slag. The alloy is water-cooled in a tank for 30 minutes, and water-cooled alloys are prone to cracking during natural cooling. To prevent rusting of the alloy during water cooling, the water cooling time should not be too long, and it should be stopped when the center is still red-hot, and the alloy will dry the remaining moisture with its own residual heat during natural cooling.
Before refining, alloy samples should be taken for analysis because ingots have segregation. Therefore, samples should be taken as follows: the ingot is evenly divided into three equal parts, and three metal columns are taken on the division line, then 4, 3, and 2 samples are taken from each column in sequence, totaling 9 samples, and then mixed evenly, with each sample weighing about 200g. The molybdenum content in the iron ingot should not deviate more than ±3%. The alloy composition has segregation, with minor deviations in carbon and sulfur, but significant deviations in molybdenum and silicon. The molybdenum content in the lower part of the ingot is more than 2% higher than that in the upper part, and the central part is slightly higher, while the silicon content in the upper and middle parts differs by about 0.7%. This indicates serious segregation. During refining, not only should the residue and internal slag on the alloy ingot be removed, but the alloy ingot should also be crushed to 40-50mm before packaging.
The standard consumption of raw materials for smelting 1t of 55% Mo ferromolybdenum is molybdenum ore (calculated based on 45% Mo, with a molybdenum recovery rate of 98.33%) 1213kg; 75% ferrosilicon 339-350kg; iron scales 250kg; steel scrap 260-270kg; aluminum granules 45-60kg; fluorite 30kg; saltpeter 40kg.
Improving molybdenum recovery is the fundamental measure to improve the economic benefits of ferromolybdenum. The main ways to lose molybdenum in production are through smoke and slag. Molybdenum in smoke mainly exists in the form of molybdenum oxide dust; molybdenum in slag mainly exists in the form of metal particles. Currently, some factories in China use large bag filters to recover molybdenum-containing dust from smelting smoke, which has achieved good results. Molybdenum in slag can be recovered by gravity separation or magnetic separation. In production, molybdenum-containing metal particles should be settled down in slag to the greatest extent possible, which requires the slag to have a low melting point and not be viscous. Therefore, the FeO content in the slag should be maintained above 16%, and the charge should have a slight excess of reducing agent and sufficient heat generation capacity.