With the extensive mining of global chromium ore resources, high-quality lump ore resources are becoming increasingly scarce, resulting in mostly fine ore after beneficiation. However, in the smelting of high carbon ferrochrome in a submerged arc furnace, an excess of fine ore deteriorates the furnace’s permeability and worsens the furnace conditions, severely impacting safety, power consumption, chromium recovery rate, and other technical and economic indicators. Consequently, the mainstream equipment, namely the fully enclosed submerged arc furnace, cannot directly use fine ore for smelting. Thus, the development of new high-carbon ferrochrome smelting processes is crucial for reducing coke powder usage and power consumption in smelting, as well as improving chromium recovery rates and market competitiveness.
Currently, the main international processes for handling and smelting fine chromium ore include the Outokumpu pelletizing and roasting method, SRC method, and DRC method.


High Carbon Ferrochrome Main Process Descriptions
1. Outokumpu Pelletizing and Roasting Method
- Chromium ore is ground, filtered, and dewatered. The ore filter cake is mixed with bentonite, pelletized, and then sent to a double-shell vertical furnace for roasting. The finished chromium ore pellets, along with coke and silica, are preheated in a rotary kiln at the top of the submerged arc furnace and then fed into a closed submerged arc furnace for smelting.
- The hot charge temperature in the submerged arc furnace is relatively low (450-550°C), making it difficult to effectively utilize physical sensible heat, resulting in higher power consumption compared to the SRC and DRC methods, about 800 kWh/t higher.
- The pellet roasting process occurs in an oxidizing atmosphere with no pre-reduction function, leading to higher coke consumption in the submerged arc furnace smelting process.
2. SRC and DRC Methods
- Both are pre-reduction methods for pellets, shifting the function of the submerged arc furnace smelting process forward by pre-reducing the pellets before entering the furnace.
- The SRC method uses a rotary kiln for pre-reduction, while the DRC method uses a rotary hearth furnace.
- The rotary hearth furnace avoids problems such as ring formation and powdering associated with the rotary kiln, effectively improving pellet quality and production efficiency.
- The rotary hearth furnace employs regenerative combustion technology, raising the internal temperature to 1400-1450°C, thereby effectively increasing the reduction rate of chromium.
New High Carbon Ferrochrome Production Method
To address the current issues of high raw material requirements, low utilization of fine ore, and high energy consumption in ferroalloy smelting, a new method for producing high-carbon ferrochrome is proposed:
1. Raw Material Handling and Preparation
- Raw materials include chromite ore fines, coke fines, and bentonite, with a carbon-to-oxygen ratio of 0.8-2.4, and bentonite constituting 1-5% of the ore weight.
- The raw materials undergo initial drying, fine grinding, and mixing, and are pelletized in a disc pelletizer. The green pellets are preheated and dried on a chain grate machine.
- After the initial drying, the moisture content of the raw materials is 1-2%; after fine grinding, the particle size of 0-0.074 mm accounts for 85-100%; the mixed material moisture content reaches 6-8% for optimal pelletizing; the green pellets have a particle size of 9-16 mm accounting for 95%, with a moisture content of 12-14%; and the moisture content of the dried pellets is 0-2%.
2. Rotary Hearth Furnace Direct Pre-reduction
- The preheated and dried pellets are fed into a rotary hearth furnace through a feeder for pre-reduction reactions, producing high-temperature direct reduced high-carbon ferrochrome pellets.
- The rotary hearth furnace is divided into zones: loading, exhaust, preheating (500-600°C), medium temperature reduction (1000-1200°C), high-temperature reduction for high-carbon ferrochrome (1350-1450°C), and discharging (800-900°C).
- The reduction time in the furnace generally ranges from 20 to 45 minutes, resulting in directly reduced high-carbon ferrochrome pellets with a metallic iron rate of 92% and a chromium metallic rate of 70%.
3. Hot Delivery System
- The high-temperature direct reduced high-carbon ferrochrome pellets (750-850°C) are transported through a hot delivery system to the submerged arc furnace bin and then charged into the furnace for deep reduction and slag-metal separation, yielding the final product.
Advantages
- Strong adaptability to raw materials and low fuel requirements, using low calorific value, and cheap gas (>800 kcal/Nm³) for the production of pre-reduced chromium ore pellets in the rotary hearth furnace.
- The pre-reduced pellets are directly hot delivered to the submerged arc furnace, effectively reducing the power consumption for smelting (2000-2200 kWh/t high-carbon ferrochrome) and the amount of reducing agent (coke fines).
- Utilizing the waste heat from the production process and the sensible heat of the pellets.
- The rotary hearth furnace avoids issues like ring formation and powdering, improving pellet quality and production efficiency, while the regenerative combustion technology increases furnace temperature, reducing energy consumption and costs, and effectively increasing the reduction rate of high-carbon ferrochrome.
This method effectively lowers the smelting power consumption and reducing agent usage, enhances pellet quality and production efficiency, and significantly improves the economic viability and competitiveness of high-carbon ferrochrome production.