Ferromolybdenum is an important alloy additive in the steel industry, and its production relies on several key raw materials, including roasted molybdenum concentrate, ferrosilicon powder, aluminum particles, mill scale, steel chips, fluorite, and sodium nitrate. The quality of these materials directly affects the quality and efficiency of ferromolybdenum production, making it essential to control both the composition and particle size of each material.


Raw Materials for Ferro molybdenum Production
1. Roasted Molybdenum Concentrate
Roasted molybdenum concentrate is the primary source of molybdenum in ferromolybdenum production, and its composition and impurity levels must meet strict requirements. The typical composition is as follows:
- Mo: 48%-52%
- S: ≤0.065%
- P: ≤0.023%
- Cu: ≤0.30%
- SiO₂: 8%-14%
- Pb: 0.2%-0.5%
In terms of particle size, the concentrate should not exceed 20mm, and particles in the 10-20mm range should account for no more than 20% of the total volume. The molybdenum in roasted concentrate is present as MoO₃, which is fully reduced to metallic molybdenum during smelting, making it the primary source of molybdenum in ferromolybdenum.
2. Ferrosilicon Powder
Ferrosilicon powder is produced by crushing and milling 75% ferrosilicon and is mainly used to reduce roasted molybdenum concentrate and other oxides. The silicon content in ferrosilicon powder typically ranges from 75%-77%. The higher silicon content is more effective in reducing the silicon content in ferromolybdenum, making it more desirable. The particle size requirements are:
- 1.0-1.8mm: no more than 1%
- 0.5-1.0mm: no more than 10%
- The remainder should be under 0.5mm.
Excessive particle size can increase the silicon content in ferromolybdenum, so controlling the particle size of ferrosilicon powder is crucial.
3. Aluminum Particles
Aluminum particles act as a reducing agent in the production of ferromolybdenum. The amount of aluminum added must be precisely controlled based on the molybdenum content of the concentrate, production scale, and other operational parameters. The aluminum content should be at least 99%, and the particle size should be no larger than 3mm. Particles that are too small can cause safety issues during production, while larger particles can hinder the smelting reaction. Typically, 5-8kg of aluminum particles are added per batch of material.
4. Mill Scale
Mill scale is the oxide layer formed during steel rolling or forging and serves as an oxidizing agent and flux during smelting. Approximately 30% of the mill scale enters the ferromolybdenum alloy, providing one source of iron, while the remaining 70% forms FeO in the slag, helping to dilute it. The composition requirements for mill scale are:
- Fe: ≥68%
- S: ≤0.05%
- P: ≤0.035%
- C: ≤0.30%
- Cu: ≤0.1%
Before use, the mill scale must be dried to remove moisture and oil. In some cases, iron ore can be used as a substitute, but due to its higher sulfur content, it is rarely used in modern production.
5. Steel Chips
Steel chips are the main source of iron in ferromolybdenum production, with a required iron content of over 98%. Carbon steel chips are commonly used.
6. Fluorite
Fluorite acts as a flux during smelting. Its particle size should be less than 20mm, and it must be dried before use to remove moisture. The composition requirements for fluorite are:
- CaF₂: ≥90%
- S: ≤0.05%
- P: ≤0.05%
The amount of fluorite added to the batch depends on the composition of the slag and the SiO₂ content in the roasted molybdenum concentrate. Typically, 2-3kg of fluorite is added per batch.
7. Sodium Nitrate
Sodium nitrate (NaNO₃) is used as a supplementary heat source when processing low-molybdenum roasted concentrates, which may lack sufficient oxygen for the reduction process. The sodium nitrate composition should be:
- NaNO₃: ≥99%
In general, 1-3kg of sodium nitrate is added per batch to increase the heat during smelting.
Batch Calculation for Ferro molybdenum Production
Based on the materials and technical conditions mentioned, a batch calculation can be performed with 100kg of roasted molybdenum concentrate as the base. The calculation parameters are as follows:
- Roasted molybdenum concentrate contains 52% Mo, while the ferromolybdenum alloy contains 60% Mo.
- Ferrosilicon powder contains 76% Si, 2% Al, and 21% Fe.
- The mill scale consists of 95% Fe₃O₄, with 30% of the iron entering the ferromolybdenum alloy and the remainder entering the slag as FeO.
- Steel chips contain 98% Fe.
- Each batch includes 20kg of mill scale, 3kg of sodium nitrate, 2kg of fluorite, and 6kg of aluminum particles (99% Al).
- The molybdenum in the roasted concentrate is present as MoO₃, which is fully reduced to metallic molybdenum.
- Sodium nitrate contains 99% NaNO₃, and the heat input must not be less than 2300 kJ/kg.
By analyzing the composition of each material and calculating the heat generation, it is possible to optimize the raw material ratios to ensure both the quality and efficiency of ferromolybdenum production.
In ferromolybdenum production, the quality and proportion of raw materials, such as roasted molybdenum concentrate, ferrosilicon powder, aluminum particles, mill scale, and steel chips, play a critical role. Through precise batch calculation and careful control of material composition, it is possible to produce high-quality ferromolybdenum while enhancing the smelting process’s stability and efficiency.
If you are interested in our ferromolybdenum, please feel free to contact us – Hongshun ferroalloy company.