High carbon silicon alloy, also known as carbon silicon alloy, is an alloy composed of silicon and carbon with a high carbon content. It is a new type of alloy used in converters and can completely replace carburizers and deoxidizers such as silicon aluminum iron. When added to molten steel, it acts as a deoxidizer, significantly improving the carbon recovery rate, which can reach over 98%. High carbon silicon alloy improves the quality of molten steel, enhances product quality, improves performance, reduces the amount of alloy added, lowers steelmaking costs, increases economic benefits, improves environmental conditions, and reduces labor intensity.


High Carbon Silicon Deoxidation Mechanism in Molten Steel
Oxygen in molten steel mainly exists in the form of ferrous oxide (FeO). If there is a high content of FeO in molten steel, it will form pores during solidification. Additionally, because FeO has high solubility in molten steel and very low solubility in solid steel, FeO will precipitate at the grain boundaries during solidification, reducing the strength and plasticity of the steel and severely damaging its mechanical properties. To avoid the adverse effects of oxygen during the steelmaking process, deoxidation treatment is necessary, usually by adding deoxidizers to the molten steel.
Advantages of High Carbon Silicon Alloy
- Strong Deoxidation Performance: With silicon content over 50%, high carbon silicon alloy has strong deoxidation ability and does not contain elements like manganese, making it widely applicable.
- High Utilization Rate: Due to its high density, high carbon silicon alloy quickly enters the molten steel to perform thorough deoxidation, improving the utilization rate of the deoxidizer.
- Cost Reduction: Compared to pure aluminum, high carbon silicon has a significantly lower production cost, and using scrap steel can further reduce costs.
- Excellent Fluidity: The high carbon content gives high carbon silicon alloy strong fluidity and filling properties during casting.
- Reliable Composition: The remelting process allows for adjustment of the alloy’s composition, ensuring reliable chemical components and avoiding harmful elements and other inclusions.
- Anti-Powdering Treatment: Treatment with an inoculant before discharge prevents the alloy from powdering easily.
Preparation Method of High Carbon Silicon Alloy
- Material Preparation and Rust Removal: Steel materials are prepared by weight, using scrap steel with an appropriate amount of ferrosilicon. Scrap steel should be shot blasted for rust removal before smelting.
- Smelting and Ingot Casting: Treated scrap steel is melted in a furnace, and when the temperature exceeds 1570℃, ferrosilicon is added. After slag removal, the molten steel is cast into ingots.
- Composition Adjustment and Remelting: The ingots are analyzed and their composition adjusted, then remelted in the furnace for further composition adjustments and slag removal.
- Addition of Anthracite and Deoxidation Treatment: When the molten steel temperature exceeds 1600℃, anthracite is added, followed by stirring, degassing, deoxidation, and inoculation treatment, then rapidly cast into shape.
Example
Using a 160KW controlled silicon medium-frequency induction furnace, the preparation process is as follows:
- Prepare 88kg of scrap steel and 1kg of 75FeSi, and shoot blast the scrap steel to remove rust.
- Melt the scrap steel in the furnace, add ferrosilicon when the temperature exceeds 1570℃.
- Remove slag and cast the molten steel into ingots.
- Analyze the ingots and adjust the composition to C 0.40%, Si 1.20%, P 0.05%, S 0.04%, Fe balance.
- Remelt the ingots in the furnace and make necessary composition adjustments.
- When the molten steel temperature exceeds 1600℃, add 71kg of anthracite after slagging and slag removal.
- Stir, degas, deoxidize, and inoculate, then rapidly cast at a temperature of 1250-1280℃.
The resulting high carbon silicon alloy deoxidizer is tested to verify its performance and composition, ensuring its effective function in the steelmaking process.