In current technology, adding graphite-like materials(Graphitized Petroleum Coke)or silicon carbide during the converter steelmaking process is a common method to compensate for temperature. The efficiency of temperature compensation with carbon additive depends on the quality of the additive and the conditions of the converter steelmaking process.


Theoretical calculations show that under the condition of a 30-ton converter semi-steel process, 1 ton of graphite-like material or silicon carbide can raise the molten steel temperature by 100-120°C. To reach temperatures above 1700°C, typically more than 500 kilograms of graphite-like material or silicon carbide are needed. However, the use of graphite-like material or silicon carbide should not exceed 10 kilograms per ton of semi-steel in the converter, as excessive use can lead to the following issues:
1. Graphite-like material:
- Low utilization rate, with some unreacted material entering the dust removal system and being wasted.
- Difficult slag formation in the early stages of steelmaking leads to “dry return” phenomena and poor phosphorus removal efficiency.
2. Silicon carbide:
- High relative cost; excessive addition can lead to slow initial slag formation and excess SiO2 in the slag, resulting in low binary basicity (CaO/SiO2) and poor phosphorus removal efficiency. Additionally, it can cause splashing during the steelmaking process.
Due to these issues, it is challenging to achieve the necessary temperatures in semi-steel steelmaking by using carbon additives for temperature compensation. Typically, the slag formation time is 3-4 minutes, and adding temperature-raising agents can delay this to 4-5 minutes. Slow slag formation directly delays the steelmaking process and may cause deep blowing, affecting the quality of the molten steel. Carbon additives are added through the scrap steel chute at the converter mouth or the top bin, which is time-consuming, labor-intensive, and increases the difficulty of operation during steel production. Therefore, the semi-steel converter steelmaking process is hard to maintain smoothly.
On the other hand, due to the high prices of primary iron and lower prices of scrap steel domestically, foundries use a high proportion of scrap steel to synthesize cast iron and directly add carbon additives in the electric furnace. However, due to different melting characteristics in the cupola, ordinary steelmaking carbon additives require temperature adjustments in the electric furnace to melt properly. Currently, available carbon additives include pig iron, pitch coke carbon additives, graphite electrode carbon additives, petroleum coke carbon additives, coal-based carbon additives, and artificial graphite carbon additives. This not only complicates the control process for foundries but also may reduce the optimal smelting time for cast iron, leading to high defect rates and low production efficiency.
To address these issues, a new type of steelmaking carbon additive has been developed. This additive has high strength, low melting point, and fast absorption speed, significantly reducing casting costs and increasing profit margins. The composition includes:
- Carbon material: 75-77.5% carbon material composed of fine graphite powder and electrode powder, with a particle size of 1200 mesh. The mass ratio of fine graphite powder to electrode powder is 55-70:50-75. Fine graphite powder comes from the processing tailings of lithium-ion battery anode graphite materials, which include natural flake graphite, petroleum needle coke artificial graphite, coal-based needle coke artificial graphite, and mesocarbon microbeads. The electrode powder is derived from waste graphite electrodes, including graphite electrodes recovered from electric furnaces used in casting, waste graphite electrodes from aluminum electrolysis, graphite cooling iron recovery materials, and waste graphite crucible materials.
- Binder: Composed of inorganic and organic binders in a mass ratio of 1:0.5-1.5. The inorganic binder includes solutions of silicic acid, silicates, and clays with pure water, with a concentration of 55-60%. The silicates include sodium silicate, potassium silicate, magnesium silicate, and calcium silicate. The organic binder is a sol of one or more of starch, carboxymethyl cellulose, sodium carboxymethyl cellulose, styrene-butadiene rubber, and polytetrafluoroethylene, with a concentration of 20-30%. The binder’s viscosity is 1200-1500 cp, and its pH is 6.5-8.0.
Preparation Steps for Steelmaking Carbon Additive
- Preparation of Carbon Material: Mix fine graphite powder and electrode powder in a mass ratio of 55-70:50-75 uniformly. Heat the mixture from room temperature to 1800-2800°C at a rate of 10-20°C/min, hold for 30 minutes, then cool naturally to room temperature and sieve through a 1200 mesh sieve to obtain the carbon material.
- Preparation of Binder: Slowly add the inorganic binder to the organic binder in a mass ratio of 1:0.5-1.5, stirring at a speed of 800-1200 rpm for 20 minutes to obtain the binder.
- Mixing: Add 2.0-5.0% of the binder to 75-77.5% of the carbon material by weight. Stir at 200-220°C for 10 minutes at a speed of 120 rpm. Continue to add iron-containing materials and stir for another 30 minutes.
- Briquetting: Use a high-pressure briquetting machine to press the mixed material into round balls. Control the pressure at 10 MPa and the roller speed of the briquette machine at 10 cm/s.
This new type of steelmaking carbon additive addresses various issues encountered with traditional additives, improving steelmaking efficiency and cast iron quality while reducing production costs.